Hajar (Guemassa, Morocco), representative: a Zn-Pb-Cu-Ag massive-sulphide concentrator with sequential lead, copper and zinc flotation
A representative model of the Hajar concentrator at Managem's Guemassa site, 35 km south of Marrakesh, at its original design point: 3,000 t/d of run-of-mine ore at 10.5% Zn, 3% Pb, 0.3% Cu and 60 g/t Ag (mining-technology.com, 'CMG Metal Mine - Hajar'). The plant there grinds in rod and ball mills and floats lead-silver, copper and zinc concentrates in sequence; this flowsheet does the same with the differential flotation model, in which every mineral of a bank has its own rate constant. The ore. Hajar is a pyrrhotite-rich massive sulphide (50-75 vol% pyrrhotite with sphalerite, galena, chalcopyrite and pyrite; Admou et al., Minerals 8:435, 2018). Here it is 60 wt% pyrrhotite (Fe7S8, the formula Marcoux et al. 2008 measured at Draa Sfar nearby), 17.5% sphalerite carrying 11.4 mol% FeS (Draa Sfar's measured mean, the same paper), 3.5% galena, 0.87% chalcopyrite, 2% pyrite and quartz for the silicate gangue. Mineral densities are webmineral's. The grades are chosen to give the design head assay exactly; the silver is placed 80% in galena and 20% in chalcopyrite (about 1,386 g/t in each), which is an assumption: a real deportment comes from mineralogy. Grinding. The mill grinds a 2.5 mm F80 to a 75 micron P80 for 1.43 MW (Bond work index 12, representative). At 400 micron grains, 72% of the galena and 76% of the sphalerite reaching the lead rougher sit in liberated particles. Flotation. Lead rougher and two cleaners (galena floats, sphalerite, pyrrhotite and chalcopyrite depressed), then copper rougher and three cleaners on the lead tailings, then the zinc rougher, scavenger and two cleaners (sphalerite activated). Each cleaner's tailings return to the stage before it and the scavenger concentrate to the zinc rougher, so the model solves seven recycles together. Particles are recovered by flotation at a rate set by their composition and by entrainment with the water: the degree of entrainment by size is Zheng, Johnson and Franzidis's measurement in a 3 m3 cell (0.56 at 7 microns, 0.18 at 25, 0.11 at 88), as reported by Ramlall (J. SAIMM 120, 2020), and the cleaners carry a froth recovery of 0.7. Magnetic cleaning of the zinc concentrate. The plant passes it through magnetic separators to reject pyrrhotite, and so does this model: a wet low-intensity separator on the last zinc cleaner's concentrate. The mineral susceptibilities are Rosenblum and Brownfield's Frantz extraction currents (USGS OFR 99-529, Table 1: pyrrhotite 0.01-0.05 A, iron-bearing sphalerite 0.60-1.00 A, chalcopyrite 0.70-1.30 A; galena, pyrite and quartz above 1.70 A) put through McAndrew's calibration K = 20 sin(15 deg)/I^2 x 1e-6 as MineralMate (Heliyon 2022) restates it, and taken as cgs: pyrrhotite 1.3e-4 m3/kg against 1.1e-7 for the sphalerite. The separator's cut (2e-5 m3/kg) and sharpness are representative. It rejects 97% of the pyrrhotite and 5.3% of the sphalerite, the sphalerite locked in pyrrhotite composites, and lifts the zinc concentrate from 47.3% to 52.5% Zn. The result, against Hajar's published figures (68% Pb at 75% recovery, 28% Cu at 70%, 52% Zn at 94%): the lead concentrate is 67.5% Pb at 75.3% recovery with 1,098 g/t Ag, the copper concentrate 27.9% Cu at 69.4%, and the zinc concentrate 52.5% Zn at 92.3%, with 10.6% Fe of which 5.8 points are the iron inside the sphalerite itself and most of the rest pyrite, which no magnetic separator removes. No published Fe assay for a Hajar concentrate was found to check that against. The tailings carry 0.09% Zn and 0.78% Pb. Each concentrate is thickened and filtered to under 10% moisture by mass, the shipping limit the mine quotes. Bounded, and stated. Every rate constant, maximum recovery and water recovery is representative, fitted here to the published grades and recoveries; none was measured on Hajar ore, and a fitted set is one of many that would match six numbers. The zinc circuit's pyrite activation in particular is a fitted value: with pyrrhotite removed magnetically, something non-magnetic must dilute the concentrate to 52% Zn. A composite particle is treated as one mineral against the average of the rest (binary composites); the unfloatable fraction (R-infinity) is redrawn in each bank rather than tracked through the circuit; and the Frantz-derived susceptibilities are screening values, a ferrimagnetic pyrrhotite at the bottom of the Frantz range being outside McAndrew's calibration.
The flowsheet
The solved topology — every unit op's real duty, conversion, or split, read straight off a genuine converged solve.
The stream table
Every stream's flow, temperature, pressure, and composition — real converged numbers, not placeholders.